E2553T1-1/4 AP Irin Alagbara Irin Flux Cored Welding Waya

Apejuwe kukuru:

E2553T1-4 AP flux-cored waya ti wa ni lilo fun didapọ duplex alagbara, irin alloys pẹlu isunmọ 25% Chromium.


Alaye ọja

ọja Tags

E2553T1-1/4 AP FLUX-Coreed WIRE

ÌSÍLẸ̀
AWS 5.22 Kilasi E2553T1-1 ati E2553T1-4 / ASME SFA 5.22 Kilasi E2553T1-1 ati E2553T1-4
UNS # W39533 A # 8 F # 6

Apejuwe
E2553T1-4 jẹ okun waya ṣiṣan ṣiṣan-gbogbo ipo ti a ṣe apẹrẹ lati ṣiṣẹ lori 75% Ar / 25% CO2.
Okun waya yii jẹ apẹrẹ lati ni yiyọ slag ti o dara julọ ati ṣiṣe pẹlu gbigbe globular ọfẹ-ọfẹ.

Awọn ohun elo
E2553T1-4 AP flux-cored waya ti wa ni lilo fun didapọ duplex alagbara, irin alloys pẹlu isunmọ 25% Chromium.
Awọn irin alagbara irin onilọpo meji wọnyi darapọ fifẹ giga ati awọn agbara ikore pẹlu imudara ilọsiwaju si pitting, ipata, ati fifọ ipata wahala.Awọn ibeere wọnyi ni igbagbogbo ni a rii ni omi okun, kemikali, ati awọn ile-iṣẹ epo.
Ti o ba nilo annealing post-weld, irin weld yii yoo nilo iwọn otutu annealing ti o ga ju eyiti o nilo nipasẹ irin ipilẹ ile olopo meji.

Ilana
Ko si preheat.Iwọn otutu interpass ti o pọju ti 300°F.
Annealing le nilo lati ṣaṣeyọri líle aṣọ-ọṣọ lori awọn alurin-ọna pupọ.
Gbigbe ooru yẹ ki o ni opin si 5-40 KJ/IN.

Aṣoju Kemistri

C Cr Ni Mo Mn Si P S N Cu
0.02 25.3 9.8 3.37 0.80 0.70 0.03 0.015 0.14 1.87

ASOJU ALAGBEKA ELEYI

LARA 25 RC bi welded 35 RC iṣẹ le
AGBARA FIFẸ 110.000 PSI min.
ÌGBÀGBÀ 15% min.

Alurinmorin parameters

ITOJU FOLTAGE AMPERAGE GAS
.045” 25-30 130-220 75% Ar / 25% CO2 tabi 100% CO2

 

Wenzhou Tianyu Itanna Co., Ltd ti dasilẹ ni ọdun 2000. A ti ṣiṣẹ ni iṣelọpọ awọn amọna alurinmorin,alurinmorin ọpá, ati alurinmorin consumables fun diẹ ẹ sii ju 20 ọdun.

Awọn ọja akọkọ wa pẹlu awọn amọna alurinmorin irin alagbara, irin alagbara, awọn elekitirodi alurinmorin, awọn amọna alurinmorin kekere, awọn ẹrọ itanna alurinmorin, awọn amọna alurinmorin nickel & cobalt alloy, awọn onirin irin kekere & kekere alloy alurinmorin, awọn irin alagbara irin alurinmorin, irin alagbara, irin alurinmorin, gaasi-dabobo flux cored wires, aluminiomu alurinmorin onirin, submerged aaki alurinmorin.wires, nickel & cobalt alloy welding wires, brass welding wires, TIG & MIG welding wires, tungsten electrodes, carbon gouging electrodes, and other welding accessories & consumables.