Nickel Alloy Welding Waya ERNiCrMo-10 Tig Waya

Apejuwe kukuru:

Nickel-chromium-molybdenum alloy ti a ṣe apẹrẹ fun didapọ C22, 625, 825 tabi awọn akojọpọ ti awọn ohun elo wọnyi.


Alaye ọja

ọja Tags

Nickel AlloyWelding WayaTig WayaERNiCrMo-10

 

 

Awọn ajohunše
EN ISO 18274 – Ni 6022 – NiCr21Mo13Fe4W3
Aws A5.14 - ER NiCrMo-10

 

Awọn ẹya ara ẹrọ ati Awọn ohun elo

Nickel-chromium-molybdenum alloy ti a ṣe apẹrẹ fun didapọ C22, 625, 825 tabi awọn akojọpọ ti awọn ohun elo wọnyi.

Pese irin weld ti ko ni Nb ti o nira fun awọn welds ti o yatọ ni Super austenitic ati Super duplex alagbara, irin.

Nfunni resistance ti o dara julọ lodi si aapọn & fifọ ipata, pitting ati ibajẹ crevice.

Ti a lo lọpọlọpọ fun awọn agbekọja ati didi awọn irin alloy kekere.

Ti a lo ni igbagbogbo ni alurinmorin ti awọn media ipata ibinu ni awọn ohun ọgbin iṣelọpọ kemikali, awọn agbekọja sooro ipata ati ni eti okun lile ati awọn agbegbe petrokemika ati bẹbẹ lọ.

Awọn iwe-ẹri idanwo le ṣee rii lori ayelujara @wilkinsonstar247.com

Awọn ohun elo Mimọ Aṣoju

Alloy 22, Alloy 625, Alloy 825, Alloy 926*
* Apejuwe, kii ṣe atokọ pipe

 

 

Iṣọkan Kemikali%

C%

Mn%

Fe%

P%

S%

Si%

Ku%

o pọju

o pọju

2.00

o pọju

o pọju

o pọju

o pọju

0.010

0.50

6.00

0.020

0.010

0.08

0.50

Ni%

ogorun

Kr%

Mo%

V%

W%

49.00

o pọju

20.00

12.50

o pọju

2.50

min

2.50

22.50

14.50

0.30

3.50

Darí Properties
Agbara fifẹ ≥690 MPa
Agbara Ikore -
Ilọsiwaju -
Agbara Ipa -

Awọn ohun-ini ẹrọ jẹ isunmọ ati pe o le yatọ si da lori ooru, gaasi idabobo, awọn aye alurinmorin ati awọn ifosiwewe miiran.

 

Awọn eefin idabobo

EN ISO 14175 - TIG: I1 (Argon)

 

Alurinmorin Awọn ipo

EN ISO 6947 - PA, PB, PC, PD, PE, PF, PG

 

Data apoti
Iwọn opin Gigun Iwọn
1.60 mm

2.40 mm

3.20 mm1000 mm

1000 mm

1000 mm5 kg

5 kg

5 kg

 